Built-up edge (BUE): what it looks like, why it happens, how to fix it
Work material stuck to the cutting edge or rake face; the surface finish turns rough and the part size drifts as the deposit grows and breaks away. Adhesion and seizure at the tool-chip interface under high contact pressure. It is not welding: there is no fusion. It forms at low cutting speed and low edge temperature on ductile, "gummy" materials such as low-carbon steel, stainless and aluminium.
| What you see | Mechanism | First fix | Most affected |
|---|---|---|---|
| Work material stuck to the cutting edge or rake face; the surface finish turns rough and the part size drifts as the deposit grows and breaks away. | Adhesion and seizure at the tool-chip interface under high contact pressure. | Raise Vc so the edge runs hotter, and use a sharp, positive PVD geometry. | ISO P (steel), ISO M (stainless steel), ISO N (non-ferrous) |
Why it happens
- Cutting speed too low: below a material-dependent range the interface is cool enough for the deposit to stay stable.
- Negative or blunt geometry raises contact pressure and gives the material somewhere to sit.
- Coating and lubricity: a coating with high affinity for the work material, or poor lubrication, promotes adhesion.
How to measure and judge it
There is no wear land to measure. The signs are a deposit visible under magnification, a torn surface finish, and size that jumps when the deposit breaks off. When it breaks off it can take carbide with it, which is why BUE is a common cause of edge chipping.
Fixes, in the order to try them
- Raise Vc. Slowing down makes BUE worse, which is the opposite of the usual instinct.
- Use a sharp, positive-rake geometry with a PVD coating suited to the material.
- Improve lubricity: coolant concentration and type matter here.
- On aluminium, inspect the corner first: a dulled corner plows instead of shearing and builds up material.
Likely causes and fixes
Each pairing below is listed under this symptom by at least two independent tool manufacturers in their published troubleshooting guides. Where the makers disagree we leave the item out.
| Likely cause | Fix | Listed by |
|---|---|---|
| Cutting zone temperature too low | Increase cutting speed | Sandvik Coromant, ISCAR, Seco Tools, Tungaloy |
| Negative geometry or a sticky, gummy work material | Use a sharper, more positive geometry | Sandvik Coromant, ISCAR, Seco Tools |
| Very sticky material (low-carbon steel, stainless steel, aluminium) | Increase coolant supply or concentration | ISCAR, Seco Tools |
Guides: Sandvik Coromant, Troubleshooting turning · ISCAR, ISO Turn Inserts Wear Troubleshooting · Seco Tools, Tool wear patterns: how to recognize and optimize them · Sandvik Coromant, Troubleshooting milling · Tungaloy, Troubleshooting in turning (Users Guide 2023-2024, L007)
Do not confuse it with
A deposit sitting in a hollow on the rake face can hide crater wear underneath. Remove it and look. See crater wear.
Other wear modes
Flank wear · Crater wear · Notch wear · Plastic deformation · Thermal cracking · Edge chipping and fracture · All eight failure modes in one table · Mechanisms in depth
Are you overpaying on your inserts? Paste your insert list and get a cost audit in about 30 seconds: cross-brand candidate alternatives at the same ISO application position, and where you are likely overpaying. No signup, no sales call.
After the free check: a sourced PDF + XLSX report from about USD 10 (EUR 9) per grade. How buying works
Frequently asked questions
What causes built-up edge on a cutting tool?
Built-up edge is caused by adhesion and seizure of work material on the edge at low cutting speed and low edge temperature, mostly on ductile materials such as low-carbon steel, stainless steel and aluminium.
Should I slow down to stop built-up edge?
No. Slowing down usually makes it worse. Raise the cutting speed so the edge runs hotter, and use a sharper, more positive geometry and better lubrication.